When you need PA6 GF30 property data, you are usually not looking for a narrative guide. You need numbers — tensile strength, flexural modulus, HDT, shrinkage — in one place, with the test standards cited so you can compare grades from different suppliers without translation errors. This page is that reference. It covers the standard property set for a heat-stabilized PA6 with 30% glass fiber reinforcement, the test methods behind each number, and the processing windows that matter to molders.

PA6 GF30 Mechanical Properties (Dry as Molded, 23 C)

속성Value (Typical Range)Test MethodUnit
Tensile Modulus9,500-10,500ISO 527-1/-2MPa
Tensile Strength at Break170-190ISO 527-1/-2MPa
휴식 시 연신율3.0-4.5ISO 527-1/-2%
굴곡 탄성 계수8,000-9,500ISO 178MPa
Flexural Strength260-290ISO 178MPa
Charpy Impact Strength (notched)12-16ISO 179/1eAkJ/m2
Charpy Impact Strength (unnotched)75-95ISO 179/1eUkJ/m2
Izod Impact Strength (notched)11-15ISO 180/AkJ/m2
Ball Indentation Hardness200-230ISO 2039-1MPa
Mechanical properties for PA6 GF30, 30% glass fiber reinforced, conditioned dry (moisture content below 0.10%). Values represent typical ranges across major commercial suppliers. Always use the supplier’s specific datasheet values for design calculations.

Thermal Properties

속성Value (Typical Range)Test MethodUnit
Melting Temperature (DSC, 10 K/min)218-222ISO 11357-1/-3C
HDT at 0.45 MPa215-220ISO 75-1/-2C
HDT at 1.8 MPa195-210ISO 75-1/-2C
Vicat Softening Temperature (VST/B50)205-215ISO 306C
Coefficient of Linear Thermal Expansion (parallel, 23-55 C)2.0-3.0 x 10-5ISO 11359-1/-21/K
Coefficient of Linear Thermal Expansion (normal, 23-55 C)6.0-9.0 x 10-5ISO 11359-1/-21/K
Thermal Conductivity0.28-0.35DIN 52612W/(m·K)
Specific Heat Capacity1.5-1.7J/(g·K)
Thermal property ranges for PA6 GF30. The CTE (coefficient of thermal expansion) is significantly anisotropic — expansion in the transverse (normal) direction is 2-4x higher than in the flow (parallel) direction due to glass fiber orientation.

Electrical Properties

속성Value (Typical Range)Test MethodUnit
Dielectric Constant (1 MHz)3.5-4.5IEC 60250
Dissipation Factor (1 MHz)0.01-0.03IEC 60250
볼륨 저항1013-1015IEC 60093ohm·cm
Surface Resistivity1012-1014IEC 60093ohm
비교 추적 인덱스(CTI)500-600IEC 60112V
Dielectric Strength (1.6 mm)30-35IEC 60243-1kV/mm
Electrical properties for standard PA6 GF30. Note: values assume dry conditioning. Moisture absorption significantly impacts electrical properties — dielectric constant and dissipation factor increase, while volume resistivity decreases by 1-2 orders of magnitude at equilibrium moisture content.

Physical Properties

속성Value (Typical Range)Test MethodUnit
밀도1.35-1.38ISO 1183g/cm3
Water Absorption (23 C, saturation)5.5-6.5ISO 62%
Water Absorption (23 C, 50% RH equilibrium)1.5-2.0ISO 62%
Molding Shrinkage (parallel, 1.6 mm)0.25-0.40ISO 294-4%
Molding Shrinkage (normal, 1.6 mm)0.80-1.10ISO 294-4%
Post-Molding Shrinkage (parallel, 1h at 110 C)0.05-0.10ISO 294-4%
Post-Molding Shrinkage (normal, 1h at 110 C)0.10-0.15ISO 294-4%
Physical properties. Note the 3:1 to 4:1 ratio between normal and parallel shrinkage — this anisotropy is the primary cause of warpage in glass-fiber-reinforced parts and must be accounted for in mold design.

Flammability

속성가치Test Method참고
UL 94 Rating (0.8 mm)HBUL 94Standard GF30 is not flame retardant
UL 94 Rating (1.6 mm)HBUL 94FR V-0 requires specialized FR compound
Limiting Oxygen Index (LOI)22-24%ISO 4589Burns in normal atmosphere
Auto-Ignition Temperature>400 CASTM D1929
Flammability properties. Standard PA6 GF30 is not self-extinguishing. For applications requiring UL 94 V-0, V-1, or V-2, a flame-retardant grade (PA6 GF30 FR) must be specified.

Processing Parameters

건조

PA6 GF30 must be dried to a moisture content below 0.10% (target 0.05%) before injection molding. Recommended drying: 80 C for 4-6 hours in a desiccant dryer with a dew point of -30 C or lower. Tray drying at 80 C for 8-12 hours is acceptable for non-critical applications but is less reliable than desiccant drying. Do not dry above 90 C — oxidative discoloration (yellowing) begins at higher temperatures.

사출 성형

ParameterRecommended Range참고
Melt Temperature (nozzle)250-280 CLower end for thin walls, upper for thick
금형 온도80-100 C100 C preferred for crystallinity and surface
Injection SpeedMedium to fastFaster fill reduces fiber orientation variation
Hold Pressure50-80% of injection pressureEnough to pack out shrinkage, avoid overpacking
Back Pressure5-15 bar (hydraulic)Higher back pressure improves melt homogeneity
Screw Speed50-150 rpmLower end for larger shot sizes to avoid shear heating
Residence Time (max at melt temp)10-15 minutesPurge if longer; degraded PA6 produces burn marks and strength loss
Injection molding parameter ranges for PA6 GF30. These are starting-point recommendations; actual parameters depend on part geometry, gate design, and machine characteristics.

Mold Design Considerations

  • Gate type: All standard gate types are suitable. Pin gates, edge gates, and fan gates all work. Tunnel (submarine) gates require attention to gate diameter — minimum 0.8 mm to avoid excessive shear with 30% GF.
  • Gate location: Position the gate so flow is into the thickest section. Avoid long flow paths that allow the melt front to cool before the cavity fills.
  • Venting: Adequate venting is critical. Poor venting leads to burn marks, short shots, and die buildup. Vent depth: 0.01-0.02 mm.
  • Draft angle: Minimum 1 degree, 2 degrees preferred for textured surfaces. GF grades shrink tightly onto cores — adequate draft prevents ejection damage.
  • Steel selection: 30% glass fiber is abrasive. For production runs exceeding 100,000 shots, use hardened tool steel (min. 52 HRC) for cavities and cores, especially at gates and high-wear areas.

Property Changes with Moisture Conditioning

PA6 absorbs moisture from the environment. At equilibrium with 50% RH at 23 C, a PA6 GF30 part will absorb approximately 1.5-2.0% water by weight. This changes the mechanical properties significantly. Tensile strength decreases by 30-40%, flexural modulus by 25-35%, and impact strength increases by 50-100%. The data table below shows the approximate shift from dry-as-molded to conditioned (50% RH) values:

속성Dry (as molded)Conditioned (50% RH, 23 C)Change
인장 강도(MPa)180110-130-30 to -40%
굴곡 탄성률(GPa)9.06.0-7.0-25 to -35%
Charpy Notched Impact (kJ/m2)1420-28+50 to +100%
HDT at 1.8 MPa (C)20065-75 (wet)Significant drop at full saturation
Approximate mechanical property shift from dry to conditioned state. Design calculations should use conditioned values if the part operates in ambient humidity. Dry values apply to parts sealed against moisture or used in very dry environments.

Comparing PA6 GF30 with Related Grades

PA6 GF30 is the most common glass-filled nylon, but it is not always the best choice. Here is how it compares numerically with neighboring grades:

속성PA6 UnfilledPA6 GF15PA6 GF30PA6 GF50PA66 GF30
인장 강도(MPa)80120-140170-190200-230180-200
굴곡 탄성률(GPa)2.85.5-6.58.0-9.514-169.0-10.5
Notched Izod (kJ/m2)5-77-1011-1513-1810-13
HDT at 1.8 MPa (C)65-75180-195195-210210-215240-255
Density (g/cm3)1.141.231.361.561.37
상대적 비용1.0x1.1x1.2x1.4x1.3x
Property comparison across PA6 glass fiber loading levels and versus PA66 GF30. PA66 GF30 delivers higher HDT (heat resistance) at similar mechanicals. PA6 GF50 provides maximum stiffness at the cost of density and impact.

About Our Engineering Plastics Supply

As an ISO 9001 certified engineering plastics manufacturer and exporter, we produce PA6 GF30 in heat-stabilized, impact-modified, UV-stabilized, and color-matched variants. Our standard grade carries UL 94 HB certification with full RoHS and REACH compliance. We supply B2B buyers worldwide with batch-specific certificates of analysis and application engineering support. For your specific requirements — whether you need a standard datasheet grade or a custom formulation — contact our technical team with your target properties and annual volume.

Need a PA6 GF30 datasheet for your application or a quotation for supply? 팀에 문의 — specify your volume, delivery destination, and any special requirements (color, certification, impact modification). We respond with datasheet and pricing within one business day.

맞춤형 솔루션 제작하기

이 필드는 필수 입력 사항입니다.
이 필드는 필수 입력 사항입니다.
이 필드는 필수 입력 사항입니다.
이 필드는 필수 입력 사항입니다.
이 필드는 필수 입력 사항입니다.
맨 위로 스크롤