When you need PA6 GF30 property data, you are usually not looking for a narrative guide. You need numbers — tensile strength, flexural modulus, HDT, shrinkage — in one place, with the test standards cited so you can compare grades from different suppliers without translation errors. This page is that reference. It covers the standard property set for a heat-stabilized PA6 with 30% glass fiber reinforcement, the test methods behind each number, and the processing windows that matter to molders.
PA6 GF30 Mechanical Properties (Dry as Molded, 23 C)
Propiedad
Value (Typical Range)
Test Method
Unit
Tensile Modulus
9,500-10,500
ISO 527-1/-2
MPa
Tensile Strength at Break
170-190
ISO 527-1/-2
MPa
Alargamiento a la rotura
3.0-4.5
ISO 527-1/-2
%
Módulo de flexión
8,000-9,500
ISO 178
MPa
Flexural Strength
260-290
ISO 178
MPa
Charpy Impact Strength (notched)
12-16
ISO 179/1eA
kJ/m2
Charpy Impact Strength (unnotched)
75-95
ISO 179/1eU
kJ/m2
Izod Impact Strength (notched)
11-15
ISO 180/A
kJ/m2
Ball Indentation Hardness
200-230
ISO 2039-1
MPa
Mechanical properties for PA6 GF30, 30% glass fiber reinforced, conditioned dry (moisture content below 0.10%). Values represent typical ranges across major commercial suppliers. Always use the supplier’s specific datasheet values for design calculations.
Thermal Properties
Propiedad
Value (Typical Range)
Test Method
Unit
Melting Temperature (DSC, 10 K/min)
218-222
ISO 11357-1/-3
C
HDT at 0.45 MPa
215-220
ISO 75-1/-2
C
HDT at 1.8 MPa
195-210
ISO 75-1/-2
C
Vicat Softening Temperature (VST/B50)
205-215
ISO 306
C
Coefficient of Linear Thermal Expansion (parallel, 23-55 C)
2.0-3.0 x 10-5
ISO 11359-1/-2
1/K
Coefficient of Linear Thermal Expansion (normal, 23-55 C)
6.0-9.0 x 10-5
ISO 11359-1/-2
1/K
Thermal Conductivity
0.28-0.35
DIN 52612
W/(m·K)
Specific Heat Capacity
1.5-1.7
—
J/(g·K)
Thermal property ranges for PA6 GF30. The CTE (coefficient of thermal expansion) is significantly anisotropic — expansion in the transverse (normal) direction is 2-4x higher than in the flow (parallel) direction due to glass fiber orientation.
Electrical Properties
Propiedad
Value (Typical Range)
Test Method
Unit
Dielectric Constant (1 MHz)
3.5-4.5
IEC 60250
—
Dissipation Factor (1 MHz)
0.01-0.03
IEC 60250
—
Resistividad volumétrica
1013-1015
IEC 60093
ohm·cm
Surface Resistivity
1012-1014
IEC 60093
ohm
Índice de Seguimiento Comparativo (ISC)
500-600
IEC 60112
V
Dielectric Strength (1.6 mm)
30-35
IEC 60243-1
kV/mm
Electrical properties for standard PA6 GF30. Note: values assume dry conditioning. Moisture absorption significantly impacts electrical properties — dielectric constant and dissipation factor increase, while volume resistivity decreases by 1-2 orders of magnitude at equilibrium moisture content.
Physical Properties
Propiedad
Value (Typical Range)
Test Method
Unit
Densidad
1.35-1.38
ISO 1183
g/cm3
Water Absorption (23 C, saturation)
5.5-6.5
ISO 62
%
Water Absorption (23 C, 50% RH equilibrium)
1.5-2.0
ISO 62
%
Molding Shrinkage (parallel, 1.6 mm)
0.25-0.40
ISO 294-4
%
Molding Shrinkage (normal, 1.6 mm)
0.80-1.10
ISO 294-4
%
Post-Molding Shrinkage (parallel, 1h at 110 C)
0.05-0.10
ISO 294-4
%
Post-Molding Shrinkage (normal, 1h at 110 C)
0.10-0.15
ISO 294-4
%
Physical properties. Note the 3:1 to 4:1 ratio between normal and parallel shrinkage — this anisotropy is the primary cause of warpage in glass-fiber-reinforced parts and must be accounted for in mold design.
Flammability
Propiedad
Valor
Test Method
Notas
UL 94 Rating (0.8 mm)
HB
UL 94
Standard GF30 is not flame retardant
UL 94 Rating (1.6 mm)
HB
UL 94
FR V-0 requires specialized FR compound
Limiting Oxygen Index (LOI)
22-24%
ISO 4589
Burns in normal atmosphere
Auto-Ignition Temperature
>400 C
ASTM D1929
—
Flammability properties. Standard PA6 GF30 is not self-extinguishing. For applications requiring UL 94 V-0, V-1, or V-2, a flame-retardant grade (PA6 GF30 FR) must be specified.
Processing Parameters
Secado
PA6 GF30 must be dried to a moisture content below 0.10% (target 0.05%) before injection molding. Recommended drying: 80 C for 4-6 hours in a desiccant dryer with a dew point of -30 C or lower. Tray drying at 80 C for 8-12 hours is acceptable for non-critical applications but is less reliable than desiccant drying. Do not dry above 90 C — oxidative discoloration (yellowing) begins at higher temperatures.
Moldeo por inyección
Parameter
Recommended Range
Notas
Melt Temperature (nozzle)
250-280 C
Lower end for thin walls, upper for thick
Temperatura del molde
80-100 C
100 C preferred for crystallinity and surface
Injection Speed
Medium to fast
Faster fill reduces fiber orientation variation
Hold Pressure
50-80% of injection pressure
Enough to pack out shrinkage, avoid overpacking
Back Pressure
5-15 bar (hydraulic)
Higher back pressure improves melt homogeneity
Screw Speed
50-150 rpm
Lower end for larger shot sizes to avoid shear heating
Residence Time (max at melt temp)
10-15 minutes
Purge if longer; degraded PA6 produces burn marks and strength loss
Injection molding parameter ranges for PA6 GF30. These are starting-point recommendations; actual parameters depend on part geometry, gate design, and machine characteristics.
Mold Design Considerations
Gate type: All standard gate types are suitable. Pin gates, edge gates, and fan gates all work. Tunnel (submarine) gates require attention to gate diameter — minimum 0.8 mm to avoid excessive shear with 30% GF.
Gate location: Position the gate so flow is into the thickest section. Avoid long flow paths that allow the melt front to cool before the cavity fills.
Venting: Adequate venting is critical. Poor venting leads to burn marks, short shots, and die buildup. Vent depth: 0.01-0.02 mm.
Steel selection: 30% glass fiber is abrasive. For production runs exceeding 100,000 shots, use hardened tool steel (min. 52 HRC) for cavities and cores, especially at gates and high-wear areas.
Property Changes with Moisture Conditioning
PA6 absorbs moisture from the environment. At equilibrium with 50% RH at 23 C, a PA6 GF30 part will absorb approximately 1.5-2.0% water by weight. This changes the mechanical properties significantly. Tensile strength decreases by 30-40%, flexural modulus by 25-35%, and impact strength increases by 50-100%. The data table below shows the approximate shift from dry-as-molded to conditioned (50% RH) values:
Propiedad
Dry (as molded)
Conditioned (50% RH, 23 C)
Change
Resistencia a la tracción (MPa)
180
110-130
-30 to -40%
Módulo de flexión (GPa)
9.0
6.0-7.0
-25 to -35%
Charpy Notched Impact (kJ/m2)
14
20-28
+50 to +100%
HDT at 1.8 MPa (C)
200
65-75 (wet)
Significant drop at full saturation
Approximate mechanical property shift from dry to conditioned state. Design calculations should use conditioned values if the part operates in ambient humidity. Dry values apply to parts sealed against moisture or used in very dry environments.
Comparing PA6 GF30 with Related Grades
PA6 GF30 is the most common glass-filled nylon, but it is not always the best choice. Here is how it compares numerically with neighboring grades:
Propiedad
PA6 Unfilled
PA6 GF15
PA6 GF30
PA6 GF50
PA66 GF30
Resistencia a la tracción (MPa)
80
120-140
170-190
200-230
180-200
Módulo de flexión (GPa)
2.8
5.5-6.5
8.0-9.5
14-16
9.0-10.5
Notched Izod (kJ/m2)
5-7
7-10
11-15
13-18
10-13
HDT at 1.8 MPa (C)
65-75
180-195
195-210
210-215
240-255
Density (g/cm3)
1.14
1.23
1.36
1.56
1.37
Coste relativo
1.0x
1.1x
1.2x
1.4x
1.3x
Property comparison across PA6 glass fiber loading levels and versus PA66 GF30. PA66 GF30 delivers higher HDT (heat resistance) at similar mechanicals. PA6 GF50 provides maximum stiffness at the cost of density and impact.
About Our Engineering Plastics Supply
As an ISO 9001 certified engineering plastics manufacturer and exporter, we produce PA6 GF30 in heat-stabilized, impact-modified, UV-stabilized, and color-matched variants. Our standard grade carries UL 94 HB certification with full RoHS and REACH compliance. We supply B2B buyers worldwide with batch-specific certificates of analysis and application engineering support. For your specific requirements — whether you need a standard datasheet grade or a custom formulation — contact our technical team with your target properties and annual volume.
Need a PA6 GF30 datasheet for your application or a quotation for supply?Contact our team — specify your volume, delivery destination, and any special requirements (color, certification, impact modification). We respond with datasheet and pricing within one business day.