Nylon Chemical Resistance: Acids, Bases, Solvents, Automotive Fluids, and Food Contact
Chemical resistance is the single most misunderstood property of nylon in engineering procurement. Most engineers treat “nylon” as a single material when assessing chemical compatibility, then are surprised when PA6 and PA12 behave dramatically differently in the same environment.
This guide provides systematic chemical resistance data for PA6, PA66, and PA12 across all major chemical classes, with clear guidance on when nylon is appropriate and when alternative materials should be specified.
Understanding Nylon Chemical Resistance Mechanisms
Nylon resistance to chemicals operates through three distinct mechanisms. Understanding which mechanism applies to your environment determines whether the material will perform reliably.
Physical resistance: The polymer matrix physically blocks chemical penetration. This is the dominant mechanism for non-polar solvents like gasoline and oils — nylon has excellent resistance because hydrocarbon molecules cannot penetrate the crystalline domains.
Chemical resistance: The polymer chain does not react with the chemical. This is why nylon is attacked by strong acids and bases — they hydrolyze the amide bonds in the polyamide chain.
Plasticization and swelling: Water and polar solvents penetrate the amorphous regions, swelling the polymer without breaking chemical bonds. This increases flexibility but reduces stiffness and dimensional accuracy.
| Chemical Class | PA6 | PA66 | PA12 | Primary Mechanism | Application Notes |
|---|---|---|---|---|---|
| Motor oils (mineral) | Превосходно | Превосходно | Превосходно | Physical barrier | Under-hood auto applications |
| Motor oils (synthetic) | Превосходно | Превосходно | Превосходно | Physical barrier | ATS, DCT fluids |
| Gasoline (aromatic) | Good (60°C) | Good (100°C) | Превосходно | Physical barrier | Fuel rails: PA66-GF30 |
| Ethanol blends (E85) | Limited | Limited (80°C) | Превосходно | Physical + swelling | Fuel lines: PA12 preferred |
| Diesel, Biodiesel | Good | Good | Превосходно | Physical barrier | Fuel system components |
| ATF / Transmission fluid | Good (120°C) | Excellent (150°C) | Good | Physical barrier | Transmission oil pans |
| Glycol coolant (50/50) | Good (100°C) | Good (130°C) | Превосходно | Swelling (limited) | Coolant reservoirs |
| Brake fluids (DOT 3/4/5) | Poor | Poor | Good | Chemical attack | Use PA12 for brake components |
| Weak acids (<10%) | Limited (elev T) | Limited (elev T) | Good | Chemical hydrolysis | PA12 or PP for acid contact |
| Strong acids (>10%) | Not recommended | Not recommended | Limited | Rapid hydrolysis | PVDF or PTFE for acid |
Water Absorption and Its Effect on Chemical Resistance
Moisture absorption fundamentally changes nylon’s chemical resistance profile. Dry nylon is more chemically resistant to polar solvents (the plasticized, wet state actually resists further polar penetration) but is more susceptible to oxidative degradation. This creates a critical design consideration: parts in wet service should be tested in the conditioned (wet) state, not dry-as-molded.
| Conditioning State | PA6 Tensile Strength | PA6 Modulus | Chemical Resistance to Water | Chemical Resistance to Acids |
|---|---|---|---|---|
| Dry as molded (0%) | 85 MPa | 3,200 MPa | N/A | Poor (brittle failure) |
| Conditioned 50% RH (2.5%) | 65 МПа | 2,000 MPa | Moderate | Moderate (ductile) |
| Saturated (9.0%) | 45-50 MPa | 1,200 MPa | Swells significantly | Moderate (ductile) |
| After drying (0.1%) | 80+ MPa | 3,000 MPa | Превосходно | Poor (brittle failure) |
Industrial and Laboratory Chemical Environments
For chemical processing and industrial equipment, verify compatibility under actual operating conditions with immersion testing. The following table provides baseline guidance for common industrial chemicals.
| Chemical | PA6 | PA66 | PA12 | Max Service Temp (°C) | Alternative Material |
|---|---|---|---|---|---|
| Sulfuric acid (10%) | Limited | Not recommended | Limited | 40°C | PVDF, HDPE |
| Hydrochloric acid (10%) | Not recommended | Not recommended | Limited | 40°C | PVDF, PTFE |
| Sodium hydroxide (50%) | Limited (>60°C) | Not recommended | Good | 80°C | PP, HDPE |
| Acetone | Limited | Not recommended | Good | 60°C | PTFE |
| Ethanol | Good | Good | Превосходно | 100°C | PA12 preferred |
| Phenol (5%) | Not recommended | Not recommended | Not recommended | N/A | PTFE only |
| Formic acid (10%) | Not recommended | Not recommended | Limited | 40°C | PTFE, PVDF |
| Calcium chloride | Limited | Limited | Good | 80°C | PA12 for salt contact |
| Steam (continuous) | Not recommended | Not recommended | Limited | 120°C | PPS, PTFE |
Automotive Fluids: The Most Common Real-World Exposure
Automotive under-hood applications define the largest volume of nylon use globally. The following data reflects ASTM D543 immersion testing results at specified temperatures and exposure durations (typically 1,000 hours = approximately 6 weeks of continuous exposure).
| Fluid | PA6 | PA66 | PA12 | Weight Change | Tensile Retention | Application Confidence |
|---|---|---|---|---|---|---|
| Engine oil SAE 5W-30 (150°C) | Превосходно | Превосходно | Превосходно | <1% | >95% | Full production use |
| Transmission fluid ATF (130°C) | Good | Превосходно | Good | <2% | >90% | Full production use |
| Power steering fluid (120°C) | Good | Good | Превосходно | <2% | >90% | Full production use |
| Coolant 50/50 EG (130°C) | Good | Good | Превосходно | <3% | >85% | Full production use |
| Brake fluid DOT 4 (120°C) | Poor | Poor | Good | >10% | <60% | PA12 only |
| Windshield washer (60°C) | Превосходно | Превосходно | Превосходно | <0.5% | >99% | Full production use |
| Battery acid (25°C) | Not recommended | Not recommended | Not recommended | N/A | N/A | PP or PE only |
| AdBlue / DEF (urea) | Good | Good | Превосходно | <1% | >95% | SCR system components |
FAQs
Q1: We need to specify a nylon for a coolant reservoir. What data do we need from our supplier?
A: Request the following for the specific coolant mixture in your application: (1) ASTM D543 weight change and tensile retention data at 130°C for 1,000 hours minimum (preferably 3,000 hours for 15-year design life), (2) the specific coolant formulation used in testing (glycol type, inhibitor package), (3) compliance with OEM specifications if required (e.g., GMW 14872 for automotive coolant circuits). PA66-GF30 is the industry standard for coolant reservoirs.
Q2: We are designing a fuel line that will contact E85 (85% ethanol) gasoline. Can nylon handle this?
A: Standard PA66 absorbs ethanol significantly, causing swelling, strength loss, and potential fuel permeation. For E85 applications, PA12 is the preferred choice — it absorbs minimal ethanol and maintains mechanical properties. PA66-GF30 with barrier layers or fluorinated inner surfaces can work but requires OEM validation. KSAN offers PA12 and barrier-grade materials for flex fuel applications.
Q3: Our parts are in a chemical cleaning environment where they contact diluted alkaline cleaners. How do we specify material?
A: PA6 and PA66 are both susceptible to alkaline hydrolysis above pH 10, particularly at elevated temperatures. PA12 offers the best resistance to alkaline cleaning agents. For critical applications, request the specific cleaning agent formulation from your end user and request a 500-hour immersion test with property retention data at the actual operating temperature.
Q4: Are the chemical resistance ratings in this guide sufficient for regulatory compliance documentation?
A: These ratings are engineering reference data for material pre-selection. For regulatory compliance (FDA food contact, EU food regulations, NSF drinking water, automotive OEM specifications), you need specific compliance test data from accredited laboratories, not generic resistance charts. KSAN provides material-specific compliance documentation packages with test reports from accredited testing laboratories for all major regulatory frameworks.