Absorção de humidade
| Condition | PA6 | PA66 |
|---|---|---|
| 50% RH | 2.7% | 2.5% |
| Saturation | 8-10% | 6-8% |
Effects
- Reduces strength and stiffness
- Increases impact resistance
- Changes dimensions
Drying Guidelines
- PA6: 80°C for 4-6 hours
- PA66: 100°C for 4-6 hours
FAQ
How do you know whether Moisture Effects on Nylon — Storage & Drying Guide fits a part?
Moisture Effects on Nylon — Storage & Drying Guide fits a part when its load capacity, temperature range, moisture exposure, wear behavior, and processing method match the real service conditions.
What properties should be checked for Moisture Effects on Nylon — Storage & Drying Guide?
Verificar a resistência, a rigidez, a resistência ao impacto, a resistência ao calor, a absorção de humidade, a estabilidade dimensional, a fricção, o desgaste e a compatibilidade química.
What is the biggest selection risk for Moisture Effects on Nylon — Storage & Drying Guide?
O maior risco é escolher a partir de um valor da folha de dados sem considerar o ambiente real, o método de processamento, a geometria da peça e a utilização a longo prazo.
When should Moisture Effects on Nylon — Storage & Drying Guide be tested before production?
Recomenda-se a realização de ensaios quando a peça é sujeita a carga, calor, produtos químicos, humidade, tolerâncias apertadas, requisitos regulamentares ou um novo ambiente de funcionamento.
Moisture Effects on Nylon — Frequently Asked Questions
Why does nylon absorb moisture?
Nylon contains amide groups that form hydrogen bonds with water.
Where can I get properly dried nylon?
Nylonplastic supplies nylon vacuum-sealed with desiccant.